化学成分 Chemical Composition
质量分数(%);下表为熔炼分析(heat analysis)限值,成品分析(product analysis)允许相应偏差。“—”表示标准未规定要求。
| 元素 Element | A | B | E | F | H | P | Q | S |
|---|---|---|---|---|---|---|---|---|
| 碳 C | 0.15–0.21 | 0.15–0.21 | 0.12–0.20 | 0.10–0.20 | 0.12–0.21 | 0.12–0.21 | 0.14–0.21 | 0.10–0.20 |
| 锰 Mn | 0.80–1.10 | 0.70–1.00 | 0.40–0.70 | 0.60–1.00 | 0.95–1.30 | 0.45–0.70 | 0.95–1.30 | 1.10–1.50 |
| 硅 Si | 0.40–0.80 | 0.15–0.35 | 0.10–0.40 | 0.15–0.35 | 0.15–0.35 | 0.20–0.35 | 0.15–0.35 | 0.15–0.40 |
| 镍 Ni | — | — | — | 0.70–1.00 | 0.30–0.70 | 1.20–1.50 | 1.20–1.50 | — |
| 铬 Cr | 0.50–0.80 | 0.40–0.65 | 1.40–2.00 | 0.40–0.65 | 0.40–0.65 | 0.85–1.20 | 1.00–1.50 | — |
| 钼 Mo | 0.18–0.28 | 0.15–0.25 | 0.40–0.60 | 0.40–0.60 | 0.20–0.30 | 0.45–0.60 | 0.40–0.60 | 0.10–0.35 |
| 硼 B | ≤0.0025 | 0.0005–0.005 | 0.001–0.005 | 0.0005–0.006 | ≥0.0005 | 0.001–0.005 | — | — |
| 钒 V | — | 0.03–0.08 | — | 0.03–0.08 | 0.03–0.08 | — | 0.03–0.08 | — |
| 钛 Ti | — | 0.01–0.04 | 0.01–0.10 | ≤0.10 | ≤0.10 | ≤0.10 | — | ≤0.06 |
| 锆 Zr | 0.05–0.15 | — | — | — | — | — | — | — |
| 铜 Cu | — | — | — | 0.15–0.50 | — | — | — | — |
| 铌 Nb,≤ | — | — | — | — | — | — | — | 0.06 |
| 磷 P,≤ | 0.025 | 0.025 | 0.025 | 0.025 | 0.025 | 0.025 | 0.025 | 0.025 |
| 硫 S,≤ | 0.025 | 0.025 | 0.025 | 0.025 | 0.025 | 0.025 | 0.025 | 0.025 |
注:成品分析(product analysis)限值较熔炼分析略宽,具体偏差按 A20/A20M 执行;订货时可按补充要求 S2 约定成品分析。锆可由铈替代,加入铈时铈/硫比按熔炼分析约为 1.5:1。铌(Columbium)与钶(Niobium)为同一元素的可互换名称。表中数值以标准正本为准。
碳 C / 锰 Mn
碳保证强度与淬透性基础;锰通过固溶强化提高强度与韧性,并改善淬透性,含量按牌号分段控制。
镍 Ni / 铬 Cr / 钼 Mo
镍改善低温韧性,铬提高强度与耐蚀性,钼提高淬透性与回火稳定性;三者配合保证调质后厚截面性能。
硼 B / 钒 V / 钛 Ti / 铌 Nb
微量硼显著提高淬透性;钒、钛、铌通过细晶与析出强化细化组织;钛还可保护硼不过度氮化。
磷 P / 硫 S
有害杂质元素,严格限量以降低冷脆、热脆与焊接裂纹倾向,提高钢的纯净度与厚板韧性。