熔炼分析 / Heat Analysis
四个牌号化学成分限值Chemical Composition Limits, wt%
下表为按公开标准文本整理的熔炼分析(heat analysis)限值;成品分析(product analysis)允许偏差按标准相应条款执行。
| 元素 Element | Grade 23 | Grade 911 | Grade 92 | Grade 122 |
|---|---|---|---|---|
| 碳 C | 0.04–0.10 | 0.09–0.13 | 0.07–0.13 | 0.07–0.14 |
| 锰 Mn | 0.10–0.60 | 0.30–0.60 | 0.25–0.66 | ≤0.70 |
| 磷 P,max | 0.030 | 0.020 | 0.020 | 0.020 |
| 硫 S,max | 0.010 | 0.010 | 0.010 | 0.010 |
| 硅 Si | ≤0.50 | 0.10–0.50 | ≤0.50 | ≤0.50 |
| 铬 Cr | 1.90–2.60 | 8.50–9.50 | 8.50–9.50 | 10.00–11.50 |
| 钼 Mo | 0.05–0.30 | 0.90–1.10 | 0.30–0.60 | 0.25–0.60 |
| 镍 Ni,max | 0.40 | 0.40 | 0.40 | 0.50 |
| 钨 W | 1.45–1.75 | 0.90–1.10 | 1.50–2.00 | 1.50–2.50 |
| 钒 V | 0.20–0.30 | 0.18–0.25 | 0.15–0.25 | 0.15–0.30 |
| 铌 Nb(Cb) | 0.02–0.08 | 0.06–0.10 | 0.04–0.09 | 0.04–0.10 |
| 氮 N | — | — | 0.025–0.075 | 0.040–0.100 |
| 硼 B | 0.0009–0.007 | — | 0.0009–0.007 | ≤0.005 |
| 铝 Al,max | 0.040 | 0.040 | 0.040 | 0.040 |
| 钛 Ti,max | 0.010 | 0.010 | 0.010 | 0.010 |
| 锆 Zr,max | 0.010 | 0.010 | 0.010 | 0.010 |
注:“—”表示该牌号在公开整理资料中未单列限值或不做规定;表中数据为工程参考,精确限值、成品分析偏差及残余元素合计要求以现行标准正本 Table 1 与供货质保书为准。
元素作用 / Element Functions
合金元素在耐热钢中的作用Why Each Element Is Added
铬 Cr提高高温抗氧化与耐蚀性,形成表面氧化膜;含量决定牌号档位。
钼 Mo固溶强化基体,提高高温蠕变强度与抗氢腐蚀能力。
钨 W以固溶方式强化并改善持久性能,是本标准区别于普通 Cr-Mo 钢的特征元素。
钒 V / 铌 Nb形成稳定碳氮化物,细化晶粒并抑制高温长期服役中的组织粗化。
氮 N在 92、122 牌号中配合钒铌析出强化,稳定马氏体/铁素体基体组织。
碳 C保证强度与淬硬倾向的平衡;含量上限直接影响焊接性与韧性。
磷 P / 硫 S杂质元素,上限受控以降低脆性与热裂倾向。
硼 B微量偏聚于晶界改善淬透性与高温性能,含量控制在很小范围内。
核对要点 / Checks
成分核对时容易忽略的条款Items Easy to Miss
熔炼与成品分析Heat vs Product Analysis
标准同时规定熔炼分析与成品分析限值;订货验收应以质保书载明的分析类别和取样位置为准。
残余元素控制Residual Elements
镍、铜、铝、钛、锆等元素有上限或合计控制要求;废料来源不明的材料应增加光谱复验。
微合金元素Microalloys
氮、硼含量区间窄,对热处理与韧性敏感;重要部件应核对熔炼报告中的实测值而非仅看牌号。
合规提示:本站成分表用于选材沟通与资料整理,不构成材料验收结论;正式设计、订货与复验须以标准正本、技术协议和第三方检验结果为准。