化学成分 Chemical Composition

质量分数(%);下表为熔炼分析(heat analysis)限值,成品分析(product analysis)允许相应偏差。“—”表示标准未规定要求。

表 2 化学成分熔炼分析要求(%,依据 SA-517/SA-517M Table 1)
元素 ElementABEFHPQS
碳 C0.15–0.210.15–0.210.12–0.200.10–0.200.12–0.210.12–0.210.14–0.210.10–0.20
锰 Mn0.80–1.100.70–1.000.40–0.700.60–1.000.95–1.300.45–0.700.95–1.301.10–1.50
硅 Si0.40–0.800.15–0.350.10–0.400.15–0.350.15–0.350.20–0.350.15–0.350.15–0.40
镍 Ni———0.70–1.000.30–0.701.20–1.501.20–1.50—
铬 Cr0.50–0.800.40–0.651.40–2.000.40–0.650.40–0.650.85–1.201.00–1.50—
钼 Mo0.18–0.280.15–0.250.40–0.600.40–0.600.20–0.300.45–0.600.40–0.600.10–0.35
硼 B≤0.00250.0005–0.0050.001–0.0050.0005–0.006≥0.00050.001–0.005——
钒 V—0.03–0.08—0.03–0.080.03–0.08—0.03–0.08—
钛 Ti—0.01–0.040.01–0.10≤0.10≤0.10≤0.10—≤0.06
锆 Zr0.05–0.15———————
铜 Cu———0.15–0.50————
铌 Nb,≤———————0.06
磷 P,≤0.0250.0250.0250.0250.0250.0250.0250.025
硫 S,≤0.0250.0250.0250.0250.0250.0250.0250.025

注:成品分析(product analysis)限值较熔炼分析略宽,具体偏差按 A20/A20M 执行;订货时可按补充要求 S2 约定成品分析。锆可由铈替代,加入铈时铈/硫比按熔炼分析约为 1.5:1。铌(Columbium)与钶(Niobium)为同一元素的可互换名称。表中数值以标准正本为准。

碳 C / 锰 Mn

碳保证强度与淬透性基础;锰通过固溶强化提高强度与韧性,并改善淬透性,含量按牌号分段控制。

镍 Ni / 铬 Cr / 钼 Mo

镍改善低温韧性,铬提高强度与耐蚀性,钼提高淬透性与回火稳定性;三者配合保证调质后厚截面性能。

硼 B / 钒 V / 钛 Ti / 铌 Nb

微量硼显著提高淬透性;钒、钛、铌通过细晶与析出强化细化组织;钛还可保护硼不过度氮化。

磷 P / 硫 S

有害杂质元素,严格限量以降低冷脆、热脆与焊接裂纹倾向,提高钢的纯净度与厚板韧性。

关键词 / Keywords