GB/T 4171-2008 牌号与熔炼化学成分
下表依据标准表 3 整理;成品钢材化学成分允许偏差按 GB/T 222 执行。数值为质量分数(%)。
| 牌号 Grade | C | Si | Mn | P | S | Cu | Cr | Ni |
|---|---|---|---|---|---|---|---|---|
| Q265GNH | ≤0.12 | 0.10~0.40 | 0.20~0.50 | 0.07~0.12 | ≤0.020 | 0.20~0.45 | 0.30~0.65 | 0.25~0.50 |
| Q295GNH | ≤0.12 | 0.10~0.40 | 0.20~0.50 | 0.07~0.12 | ≤0.020 | 0.25~0.45 | 0.30~0.65 | 0.25~0.50 |
| Q310GNH | ≤0.12 | 0.10~0.40 | 0.25~0.75 | 0.07~0.12 | ≤0.020 | 0.20~0.50 | 0.30~1.25 | ≤0.65 |
| Q355GNH | ≤0.12 | 0.20~0.75 | ≤1.00 | 0.07~0.15 | ≤0.020 | 0.25~0.55 | 0.30~1.25 | ≤0.65 |
| Q235NH | ≤0.13 | 0.10~0.40 | 0.20~0.60 | ≤0.030 | ≤0.030 | 0.25~0.55 | 0.40~0.80 | ≤0.65 |
| Q295NH | ≤0.15 | 0.10~0.50 | 0.30~1.00 | ≤0.030 | ≤0.030 | 0.25~0.55 | 0.40~0.80 | ≤0.65 |
| Q355NH | ≤0.16 | ≤0.50 | 0.50~1.50 | ≤0.030 | ≤0.030 | 0.25~0.55 | 0.40~0.80 | ≤0.65 |
| Q415NH | ≤0.12 | ≤0.65 | ≤1.10 | ≤0.025 | ≤0.030 | 0.20~0.55 | 0.30~1.25 | 0.12~0.65 |
| Q460NH | ≤0.12 | ≤0.65 | ≤1.50 | ≤0.025 | ≤0.030 | 0.20~0.55 | 0.30~1.25 | 0.12~0.65 |
| Q500NH | ≤0.12 | ≤0.65 | ≤2.0 | ≤0.025 | ≤0.030 | 0.20~0.55 | 0.30~1.25 | 0.12~0.65 |
| Q550NH | ≤0.16 | ≤0.65 | ≤2.0 | ≤0.025 | ≤0.030 | 0.20~0.55 | 0.30~1.25 | 0.12~0.65 |
备注:a) 可添加微量合金元素 Nb 0.015%~0.060%、V 0.02%~0.12%、Ti 0.02%~0.10%、Alt≥0.020%,组合使用时至少一种达到下限;b) 可添加 Mo≤0.30%、Zr≤0.15%;c) Nb、V、Ti 总量不应超过 0.22%;d) 供需协商后 S 可不大于 0.008%;e) 协商后 Ni 下限可不作要求;f) 协商后 C 可不大于 0.15%。
TB/T 1979-2023 常规与冷轧牌号化学成分(节选)
| 牌号 Grade | C | Si | Mn | P | S | Cu | Cr | Ni | 其他 Others |
|---|---|---|---|---|---|---|---|---|---|
| Q295NQR2 | ≤0.12 | 0.10~0.40 | 0.20~0.50 | 0.060~0.120 | ≤0.020 | 0.25~0.45 | 0.30~0.65 | 0.25~0.50 | — |
| Q295NQR3 | ≤0.12 | 0.20~0.40 | 0.25~0.55 | 0.060~0.120 | ≤0.020 | 0.25~0.50 | — | — | Ti≤0.030;RE 0.010~0.040 |
| Q345NQR2 | ≤0.12 | 0.25~0.75 | 0.20~0.50 | 0.060~0.120 | ≤0.020 | 0.25~0.50 | 0.30~1.25 | 0.12~0.65 | — |
| Q345NQR3 | ≤0.12 | 0.20~0.50 | 0.25~0.70 | 0.060~0.120 | ≤0.020 | 0.25~0.50 | — | — | Ti≤0.030;RE 0.010~0.040 |
| Q345NQR4 | ≤0.12 | 0.20~0.40 | 0.20~0.50 | 0.060~0.120 | ≤0.020 | 0.25~0.50 | — | — | V 0.020~0.080;RE 0.010~0.040 |
| Q400NQR1 | ≤0.12 | ≤0.75 | ≤1.10 | ≤0.025 | ≤0.008 | 0.25~0.55 | 0.30~1.25 | 0.12~0.65 | — |
| Q265NQL2 | ≤0.12 | 0.10~0.40 | 0.20~0.50 | 0.060~0.120 | ≤0.020 | 0.25~0.45 | 0.30~0.65 | 0.25~0.50 | — |
| Q310NQL2 | ≤0.12 | 0.25~0.75 | 0.20~0.50 | 0.060~0.120 | ≤0.020 | 0.25~0.50 | 0.30~1.25 | 0.12~0.65 | — |
新增 N(M)、高耐蚀 EW、耐酸 AW 牌号化学成分(节选)
| 牌号 Grade | C | Si | Mn | P | S | Cu | Cr | Ni | 其他 Others |
|---|---|---|---|---|---|---|---|---|---|
| Q355NQN(M)1 | ≤0.12 | ≤0.50 | 0.50~1.50 | ≤0.030 | ≤0.015 | 0.25~0.55 | 0.40~0.80 | ≤0.65 | — |
| Q355NQN(M)6 | 0.05~0.12 | 0.20~0.40 | 0.80~1.60 | ≤0.030 | ≤0.006 | 0.25~0.40 | 0.35~0.85 | 0.15~0.65 | Ti≤0.120;V≤0.120 |
| Q350EWR1 | ≤0.07 | ≤0.50 | ≤1.10 | ≤0.020 | ≤0.010 | 0.30~0.55 | 3.00~5.50 | 0.10~0.65 | — |
| Q450EWR1 | ≤0.07 | ≤0.50 | ≤1.50 | ≤0.020 | ≤0.010 | 0.30~0.55 | 3.00~5.50 | 0.10~0.65 | — |
| Q350EWL1 | ≤0.07 | ≤0.50 | ≤1.10 | ≤0.020 | ≤0.010 | 0.30~0.55 | 3.0~5.50 | 0.10~0.65 | — |
| Q350AWR5 | ≤0.12 | ≤0.50 | ≤1.10 | ≤0.020 | ≤0.010 | 0.25~0.55 | 0.30~1.25 | 0.10~0.65 | Sb 0.020~0.300 |
| Q450AWR5 | ≤0.12 | ≤0.50 | ≤1.50 | ≤0.020 | ≤0.010 | 0.25~0.55 | 0.30~1.25 | 0.10~0.65 | Sb 0.020~0.300 |
| Q550AWR5 | ≤0.16 | ≤0.75 | ≤2.00 | ≤0.020 | ≤0.010 | 0.25~0.55 | 0.30~1.25 | 0.10~0.65 | Sb 0.020~0.300 |
| Q310AWL5 | ≤0.12 | ≤0.50 | ≤1.10 | ≤0.020 | ≤0.010 | 0.25~0.55 | 0.30~1.25 | 0.10~0.65 | Sb 0.020~0.300 |
| Q350AWL5 | ≤0.12 | ≤0.50 | ≤1.10 | ≤0.020 | ≤0.010 | 0.25~0.55 | 0.30~1.25 | ≤0.65 | Sb 0.020~0.300 |
碳当量控制:Q355NQN(M)1 与 Q355NQN(M)6 为满足焊接性,碳当量 CE = C + Mn/6 + (Cr+Mo+V)/5 + (Ni+Cu)/15 应小于 0.45。1 类和 2 类钢加入 V、Nb、Ti 等微合金元素时,加入总量不应超过 0.220%。
成分类别设计思路
2 类 Cu-P-Cr-Ni
以 Cu、P 为核心耐候元素,配 Cr、Ni 稳定锈层,代表 Q295NQR2 / Q345NQR2 / Q310NQL2;磷控制在 0.060%~0.120%,硫≤0.020%。
3 类 Cu-P-Ti-RE
以 Ti 微合金化配合稀土(RE)净化、球化夹杂,使磷分布均匀,代表 Q295NQR3 / Q345NQR3。
4 类 Cu-P-V-RE
以 V 析出强化配合 RE,代表 Q345NQR4(对应老牌号 08CuPVRE)。
1 类 Cu-Cr-Ni
低磷低硫、高洁净度路线,代表 Q400NQR1 及高强、高耐蚀牌号。
5 类 Cu-Cr-Ni-Sb
加入 Sb 改善耐酸腐蚀性能,用于酸性 / 含硫较强环境,代表 AW 系牌号。
6 类 Cu-Cr-Ni-微钛铌钒锆
以 Nb/V/Ti/Zr 微合金化配合控轧控冷,代表 Q355NQN(M)6。
提示:高磷体系对焊接性与低温韧性较敏感,重要接头宜进行焊接工艺评定;完整牌号行与全部成分限值以标准正式版表 2 为准。