A709/A709M-26 · 桥梁结构钢 Structural Steel for Bridges
A709 桥梁钢A709 Bridge Steel
成排钢板板面 Plate surfaces in rows
Mechanical Properties · 力学与冲击

力学性能与冲击韧性

Mechanical Properties and Notch Toughness

Rp0.2 250–690 MPaCVN 分区 Zone 1–3T / F 双标识
首页 Home/标准体系/力学性能与冲击韧性

桥梁钢的力学指标要分两层看:室温拉伸决定承载能力,冲击韧性决定低温与动载下的抗脆断能力。A709 把后者写成了可执行的表格——按构件类型分 T/F,按服役温度分 Zone,按厚度分档,三者交叉查表才能得出一个可验收的数值。

Two layers matter: room-temperature tension for load capacity, and notch toughness for brittle fracture resistance. A709 turns the latter into tables indexed by member type (T/F), service temperature zone and thickness.

01

拉伸性能

Tensile properties
左右滑动查看完整表格 · Swipe horizontally for the full table
牌号 Grade屈服 MPa抗拉 MPa8 in. 伸长率2 in. 伸长率备注
36 [250]250400–5502023抗拉区间 400–550 MPa,塑性与韧性储备较充裕
50 [345]345450 min1821抗拉仅设下限,与欧标上限体系不同
50S [345S]345450 min1821屈服设 345–450 MPa 区间,屈强比 ≤0.85/0.87
QST 50 [QST 345]345450 min1821以型钢供货,表面快冷后自回火,STT 595–705 ℃
QST 50S [QST 345S]345450 min1821屈服区间 345–450 MPa,屈强比 ≤0.85/0.87
50W [345W]345485 min1821耐候指数 ≥6.0(G101),可裸用
HPS 50W [HPS 345W]345485 min1821C ≤0.11%,S ≤0.006%,钙处理控制硫化物形态
50CR [345CR]345485 min1821Cr 10.5–12.5%,可裸用,对应 A1010/A1010M
QST 65 [QST 450]450550 min1517屈服 450 MPa 级型钢,适合短跨重载
QST 70 [QST 485]485620 min1416屈服 485 MPa 级型钢,减薄效果明显
HPS 70W [HPS 485W]485585–760—19抗拉 585–760 MPa,2 in. 伸长率 19%
HPS 100W [HPS 690W]690760–895—18>65–100 mm 屈服降至 620 MPa,抗拉 690–895 MPa

依据表 1;HPS 100W 厚度 >65–100 mm 时屈服降至 620 MPa、抗拉 690–895 MPa。Per Table 1; HPS 100W properties step down above 65 mm.

02

折减与屈强比

Adjustments and yield ratio

两条折减规则必须记住。其一,钢板宽度超过 600 mm 时,伸长率要求下调 2 个百分点;其二,型钢翼缘厚度超过 75 mm 时,Grade 50 的 2 in. 伸长率按 19% 判定。折减只针对塑性指标,屈服与抗拉的下限不因尺寸放宽。

50S 与 QST 50S 另设屈强比上限:腹板取样时不超过 0.87,其他位置不超过 0.85。屈强比过高意味着材料在屈服后很快进入强化段,抗震与抗疲劳储备不足;这也是 50S 与普通 50 的核心区别之一。

Grade 36 有一个例外:截面积小于 1 in.²(645 mm²)的型钢与厚度小于 12.5 mm 的非扁钢棒材,制造厂可不做拉伸试验。这条豁免只适用于小规格,不能推广到大规格产品。

03

服役温度分区

Service temperature zones
左右滑动查看完整表格 · Swipe horizontally for the full table
分区 Zone最低服役温度 Minimum service temperature典型地区 Reference
Zone 10 ℉ [−18 ℃] 及以上温和气候、无严寒记录地区
Zone 2低于 0 ℉ 至 −30 ℉ [−18 至 −34 ℃]冬季低温但极端值有限的地区
Zone 3低于 −30 ℉ 至 −60 ℉ [−34 至 −51 ℃]高寒地区、山区与北部内陆

分区按最低服役温度确定,试验温度随之变化。Zones follow minimum service temperature; test temperature follows the zone.

04

非断裂控制构件(T 类)

Non-fracture-critical members (T)
左右滑动查看完整表格 · Swipe horizontally for the full table
牌号厚度 mmZone 1Zone 2Zone 3
36T [250T]≤10015 [20] @ 21 ℃15 [20] @ 4 ℃15 [20] @ −12 ℃
50T [345T]≤5015 [20] @ 21 ℃15 [20] @ 4 ℃15 [20] @ −12 ℃
50ST [345ST]50–10020 [27] @ 21 ℃20 [27] @ 4 ℃20 [27] @ −12 ℃
HPS 50WT≤10020 [27] @ −12 ℃20 [27] @ −12 ℃20 [27] @ −12 ℃
QST 65T [450T]≤5020 [27] @ 10 ℃20 [27] @ −7 ℃20 [27] @ −23 ℃
QST 70T [485T]≤5020 [27] @ 10 ℃20 [27] @ −7 ℃20 [27] @ −23 ℃
HPS 70WT≤10025 [34] @ −23 ℃25 [34] @ −23 ℃25 [34] @ −23 ℃
HPS 100WT≤6525 [34] @ −34 ℃25 [34] @ −34 ℃25 [34] @ −34 ℃

表中数值为三个试样的平均吸收能量,单位 ft-lbf [J] 与试验温度。Minimum average energy, ft-lbf [J] at the stated temperature.

05

断裂控制构件(F 类)

Fracture-critical members (F)
左右滑动查看完整表格 · Swipe horizontally for the full table
牌号厚度 mmZone 1Zone 2Zone 3
36F [250F]≤10025 [34] @ 21 ℃25 [34] @ 4 ℃25 [34] @ −12 ℃
50F [345F]≤5025 [34] @ 21 ℃25 [34] @ 4 ℃25 [34] @ −12 ℃
50SF [345SF]50–10030 [41] @ 21 ℃30 [41] @ 4 ℃30 [41] @ −12 ℃
HPS 50WF≤10030 [41] @ −12 ℃30 [41] @ −12 ℃30 [41] @ −12 ℃
QST 65F≤5030 [41] @ 10 ℃30 [41] @ −7 ℃30 [41] @ −23 ℃
QST 70F≤5030 [41] @ 10 ℃30 [41] @ −7 ℃30 [41] @ −23 ℃
HPS 70WF≤10035 [48] @ −23 ℃35 [48] @ −23 ℃35 [48] @ −23 ℃
HPS 100WF≤6535 [48] @ −34 ℃35 [48] @ −34 ℃35 [48] @ −34 ℃

F 类另设单值下限(如 50F 为 20 ft-lbf [27 J]),平均值与单值须同时满足。F grades also carry a minimum single-value requirement.

06

硬度、复验与试验频次

Hardness, retest and frequency

HPS 100W 除拉伸与冲击外,还须做布氏硬度试验,具体指标按表 1。硬度用于辅助判断调质工艺是否稳定,不能代替拉伸判定。

冲击试验频次按 A673/A673M 的 H 或 P 频次执行:T 类多为 H 频次,F 类与 HPS 系列多为 P 频次。F 类钢板的取样位置更密——轧态与控轧板在每张板的两端取样,正火板在一端取样,调质板在两端取样。频次与位置写错,整套冲击数据在监理审核时都可能被判无效。

复验规则分两类:普通牌号按 A6/A6M 复验;调质钢板可在重新热处理后复验,但全部力学性能须重做,不能只补做不合格项。

温度补偿条款:当实测屈服强度高于标准下限 15 ksi(105 MPa)以上时,冲击试验温度可按每超出 10 ksi(70 MPa)降低 8 ℃,具体分档见标准表 11、表 12 脚注。A temperature adjustment applies when actual yield exceeds the specified minimum by 15 ksi or more.